In the construction of glass melting furnace, there are two kinds of zirconium ramming materials commonly used, namely zircon ramming and electrofusion AZS enamelling, although both zirconium ramming materials have good anti-glass. Liquid erosion performance, only very low pollution to glass, but still need to use

"/>

同性男男黄g片免费网站丨亚洲精品国产精品乱码视色丨极品国产在线丨在线视频观看一区丨国产99在线 | 欧洲丨亚洲αv无码一区二区三区四区丨一级黄av丨狠狠躁夜夜躁人人爽超碰女h丨欧美精品一丨国产一卡二卡三卡四卡丨日韩在线视频一区二区三区丨亚洲国产欧美日韩在线丨91免费视频网站丨91黄色免费看丨国产一区二区精品久久丨国产成人av综合久久丨天堂中文在线8丨天天色播丨亚洲国产成人精品久久久国产成人丨777777av丨五十路熟妇高熟无码视频丨另类捆绑调教少妇丨在线看免费无码av天堂的丨激情六月色丨一区二区三区av夏目彩春

NEWS

news

Time:2019-10-29 16:11:32Browse volume:

In the construction of glass melting furnace, there are two kinds of zirconium ramming materials commonly used, namely zircon ramming and electrofusion AZS enamelling, although both zirconium ramming materials have good anti-glass. Liquid erosion performance, only very low pollution to the glass, but still need to be properly selected according to the nature of the glass produced.


 The ramming material consists of a gas phase, a crystal phase and a glass phase. Although the presence of the glass phase is advantageous for sintering, it is less resistant to corrosion of the glass liquid than the crystal phase, and is a weak link for the erosion resistance of the ramming material and other refractory materials. The nature and content have an important influence on the performance of the ramming material.


The pores are the channels through which the glass liquid penetrates into the ramming material. The porosity is high, and the ramming material is resistant to chemical corrosion. This is because the pores are mostly concentrated in the bonding phase. Once the glass liquid penetrates into the ramming material, the gas phase, the glass phase and The etchant meets in multiple phases, forming a weak point against erosion. Therefore, if the chemical composition is constant, the lower the total porosity, the stronger the erosion resistance.


The type and composition of the etchant also plays a large role in the erosion resistance of the ramming material. In glass kiln, the etchant mainly refers to the high temperature glass liquid and the dense metal or metal oxide deposited on the bottom of the pool. Different glass solutions have different effects on the ramming material. The characteristic rate of erosion and the form of erosion are very different between soda-lime-silica glass, borosilicate glass, lead glass and other types of glass.


The main difference between fused AZS ramming and zircon ramming is the content of Al2O3 and porosity. Since there is a masonry gap in the paving brick located on the upper layer of the zirconium ramming material, the glass liquid will penetrate into the ramming layer through the brick joint, and the erosion resistance of the ramming material will be due to the chemical composition, moving speed and temperature of the glass liquid. Different. The soda-lime-silica glass melt is highly aggressive due to the ionized alkali in the melt, and the ionized alkali is the driving force of the corrosion mechanism when they are in contact with the ramming material. The viscosity of the melt also has a large effect on the rate of erosion, regardless of which glass system is in the range, and the erosion increases sharply with decreasing viscosity.


The following is a further explanation of the action occurring when zircon ramming and electrofusion AZS granules are in contact with alkaline glass.


(1) The fused AZS ramming material is in contact with the alkaline glass liquid, and the aluminum (Al2O3) layer is formed at the contact interface. The ZrO2 in the ramming material is melted in the glass liquid to a low degree, the viscosity is increased, and the interface layer is blunt. Chemical properties, anti-mechanical wear and chemical resistance.


(2) The zircon ramming material is in contact with the alkaline glass liquid. Since the zircon ramming material has no aluminum, the zircon is easily decomposed, and the decomposed SiO2 reduces the viscosity, thereby accelerating the erosion. Causes damage to the beating layer.